C93700 High-Leaded Tin Bronze is also known as SAE 64 and 80-10-10 Bronze. The lead found in CDA 937 Tin Bronze acts as a lubricant and contributes to this alloys excellent machinability and good anti-friction properties. C93700 has reasonable corrosion resistance to seawater and brine and good overall wear resistance. C937 Bronze is available as centrifugal cast, continuous cast and sand cast bar. CDA 937 High-Leaded Tin Bronze is ideally suited for high speed, light duty applications, including crank shafts, washers, bushings, bearings, bearing plates and pump impellers.
Available in rounds & tube. Also cast to size.
Specifications for C93700
ASTM | |
Rounds/tubes | ASTM B505 |
sand cast | ASTM B584 |
centrifugal | ASTM B271 |
All Methods | QQ-C390 |
Mechanical Properties for for C93700
tensile | Yield | Elongation | |
Centrifugal | 30 min. | 12 min. | 15% |
Continuous Cast | 35 min. | 20 min. | 6% |
sand cast | 30 min | 12 min. | 15% |
Compositions for C93700 High Leaded Tin Bronze
UNS No. | Copper | Tin | Lead | Zinc | Nickel incl. Cobalt | Iron | Aluminum | Antimony | Sulfur | Phosphorus | Silicon |
C93700 | 78.0-82.0 | 9.0-11.0 | 8.0-11.0 | 0.8 max | 0.50 max | 0.70 max | 0.005 | 0.50 max | 0.08 max | 1.5 max |
0.005 max
|
Physical Properties of C93700
Physical Properties View Metric Conversions Table
|
Melting Point – Liquidus°F
|
1705 |
Melting Point – Solidus°F
|
1403 |
Densitylb/cu in. at 68°F
|
0.32 |
Specific Gravity
|
8.86 |
Electrical Conductivity% IACS at 68°F
|
10 |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F
|
27.1 |
Coefficient of Thermal Expansion 68-39210⁻⁶ per °F (68 – 392°F)
|
10.3 |
Specific Heat CapacityBtu/ lb /°F at 68°F
|
0.09 |
Modulus of Elasticity in Tensionksi
|
11000 |
Incipient Melting°F
|
600 |
Magnetic Permeability
|
1 |
Applications for C93700 High Leaded Tin Bronze
Bushings |
Bearings |
Wearplates
|
Impellers |
Pump Parts
|
Marine Products
|
Valves |
Rolling Mill Bearings
|
Hydraulic Press Main Liners
|
Hydraulic Press Stuffing Box
|
Thrust Washers
|
TrunionBearings
|